Austin Gallery

Reference · Updated November 2026

Earthenware vs stoneware vs porcelain

The three clay families compared on the numbers that decide what a pot can do: firing cone, water absorption, shrinkage and strength, with the definitions behind each line.

By · Published November 17, 2026

Earthenware is fired around cone 010 to 04 (1657 to 1945°F) and stays porous, absorbing more than 3% of its dry weight in water. Stoneware is fired around cone 5 to 10 (2167 to 2345°F) and absorbs 3% or less. Porcelain is a fine white body fired hot enough to absorb 0.5% or less. The 3% and 0.5% lines are the US International Trade Commission definitions, cited by Dave Finkelnburg in Ceramics Monthly and measured with the ASTM C373 boil test. Firing temperature gets a clay to its line; the absorption number is the proof that it got there.

The 3 percent line

Most comparisons describe the three families by color and feel. The definitions that actually separate them are absorption numbers. Under the USITC wording Finkelnburg quotes, stoneware is a fired ceramic that can absorb no more than 3% of its dry weight of water, earthenware absorbs more than 3%, and porcelain absorbs no more than 0.5% under the same test. The test itself is strict: five fully dry samples of at least 10 g each are boiled for 5 hours in deionized water, left to cool in it for 24 hours, blotted, and weighed.

That makes the 3 percent line a practical rule for anyone making functional work. A mug that is above 3% is not finished stoneware, whatever the bag says. Finkelnburg gives the other end too: stoneware fired to significantly less than 1.5% absorption is likely overfired, which is where slumping and bloating begin.

Side-by-side comparison

ClayCone°F°CAbsorptionShrinkageStrengthTypical uses
EarthenwareCone 010 to 041657 to 1945°F903 to 1063°CMore than 3%; buff and white bodies often 10% or moreAbout 6% to 12%Weakest, but best thermal shock resistanceTerra cotta, planters, majolica, slip-decorated ware, decorative pieces
StonewareCone 5 to 102167 to 2345°F1186 to 1285°C3% or less when matureAbout 11.5% to 15%Strong and durable; less dense than porcelainEveryday mugs, bowls, plates, bakeware, production pottery
PorcelainUsually cone 6 to 102232 to 2345°F1222 to 1285°C0.5% or lessAbout 13% to 14.75%Strongest when fully vitrified; prone to warpingFine tableware, translucent pieces, technical ceramics

Cone ranges: earthenware per Digitalfire; stoneware is the common studio range; porcelain per Digitalfire's note that it is usually fired above 1180°C. Temperatures are Orton self-supporting cones at 108°F (60°C) per hour, from our kiln cone temperature chart. Absorption lines are the USITC definitions. Shrinkage ranges come from manufacturers' published specs for named bodies, collected in our clay shrinkage and absorption chart. Strength notes follow Digitalfire.

What the manufacturers publish

A family name is a starting point. The numbers belong to a specific body at a specific cone, and the same bag of clay can land on either side of the 3 percent line depending on how hard it is fired.

Clay bodyTypeFired toShrinkageAbsorption
AMACO No. 38 White StonewareStonewareCone 513%7%
AMACO No. 38 White StonewareStonewareCone 1015%1.4%
AMACO No. 77 Terra CottaTerra cotta, fired highCone 510.5%0.9%
Laguna #550 Porcelain (WC631)PorcelainCone 1014.75%0.3%

Published specs: AMACO No. 38, AMACO No. 77, Laguna #550. More bodies, including Standard Clay earthenwares, are in our shrinkage and absorption chart.

Earthenware

Digitalfire defines earthenware as clay fired at low temperatures, cone 010 to 04, made from natural clays that do not vitrify there. The particles bond by sintering rather than melting together, so the body stays porous. Most people picture red terra cotta, but buff and white low-fire bodies belong here too, and Digitalfire notes they often absorb 10% or more.

The tradeoff is strength for forgiveness. Earthenware is the weakest of the three and chips more easily, but its porosity makes it resistant to thermal shock, and it avoids what Digitalfire lists among stoneware's drawbacks: dramatically higher firing costs. It is the natural surface for slip decoration at leather-hard and for bright low-fire glazes. Functional earthenware depends on its glaze to hold liquid.

Stoneware

Digitalfire describes stoneware, as potters use the word, as high-temperature, non-white bodies fired dense enough to make functional ware that is strong and durable, traditionally around 1200°C and up. In a US studio that usually means cone 5 to 6 in an electric kiln or cone 10 in a gas kiln. Stoneware is the default body for production pottery partly because it is forgiving in the studio: Digitalfire notes it produces fewer drying cracks than porcelain.

Mid-range and high-fire stoneware are not interchangeable

A stoneware rated cone 10 that is fired to cone 6 is underfired. AMACO's No. 38 White Stoneware is the clearest public example: AMACO publishes 7% absorption at cone 5 and 1.4% at cone 10. At the bottom of its own range that body is more than twice the 3 percent line. Check the absorption figure at your cone, not just the range printed on the box.

Porcelain

Digitalfire describes traditional porcelain as a white-burning, vitreous body of feldspar, clay and quartz, made from fine-grained materials that lack the iron impurities of stoneware, and usually fired above 1180°C. Well-vitrified porcelains low in titanium can be translucent. The cost of that glassiness is movement: the closer a body is fired to melting, the more it tends to warp, and porcelain shrinks the most of the three. Laguna publishes 14.75% shrinkage and 0.3% absorption for its #550 cone 10 porcelain.

Exceptions and distinctions

Free to use

Put this clay comparison chart on your site

Teaching an intro ceramics class or writing a studio guide? Copy the snippet below to embed the summary chart. It is self-contained and renders anywhere. The only ask is that you keep the small credit link back here.

Click inside the box, select all (⌘A / Ctrl-A), and copy.

Sources

Questions

What is the difference between earthenware, stoneware and porcelain?

Firing temperature and how much water the fired clay absorbs. Earthenware is fired around cone 010 to 04 (1657 to 1945°F) and stays porous, absorbing more than 3% of its weight in water. Stoneware is fired around cone 5 to 10 (2167 to 2345°F) and absorbs 3% or less. Porcelain is a white, fine-grained body fired hot enough to absorb 0.5% or less. The 3% and 0.5% lines are the USITC definitions cited in Ceramics Monthly.

Which is stronger, stoneware or porcelain?

Fully vitrified porcelain is generally stronger and denser than stoneware. Digitalfire describes stonewares as having lower fired strength than porcelains because they are less dense, while noting that a good glaze brings stoneware close to porcelain strength. In practice a well-fired stoneware mug and a porcelain mug are both durable; earthenware is the one that chips more easily.

Is earthenware waterproof?

Not by itself. Earthenware is fired below the point where its particles fuse, so the body stays porous, often 10% or more absorption for buff and white low-fire bodies according to Digitalfire. A sound glaze makes the surface watertight. Unglazed terra cotta planters wick water on purpose, which is why they dry out faster than glazed pots.

What temperature is stoneware fired at?

Studio stoneware is usually fired at cone 5 to 6 (2167 to 2232°F, 1186 to 1222°C) in electric kilns, or cone 10 (2345°F, 1285°C) in high-fire kilns, using Orton's self-supporting cone temperatures at 108°F per hour. Digitalfire gives the traditional threshold as about 1200°C and up. What matters is that the body reaches 3% absorption or less at the cone you actually fire.

Why does porcelain shrink more than stoneware?

Porcelain is made of fine-grained materials fired close to melting, so more of the body turns to glass and the particles pack tighter. Laguna publishes 14.75% shrinkage for its #550 cone 10 porcelain, compared with 13% for AMACO No. 38 stoneware at cone 5. Size porcelain pieces larger at the wheel and expect more warping on wide, flat forms.

Which clay is best for mugs and dinnerware?

Stoneware or porcelain fired to maturity, meaning 3% absorption or less for stoneware and 0.5% or less for porcelain. Dave Finkelnburg notes in Ceramics Monthly that vessels made of underfired clays will leak. Earthenware dinnerware works when the glaze is sound, but it chips more easily and depends on the glaze to hold liquid.

Can earthenware handle temperature changes better than stoneware?

Often, yes. Its porosity gives it good thermal shock resistance. In a Digitalfire flame test, a glazed terra cotta cup survived 25 seconds of direct flame, compared with about 10 seconds for typical stonewares and porcelains and 5 seconds for super-vitreous porcelains. Porosity trades strength for that resistance.

Keep reading

Absorption definitions are the USITC wording as cited in Ceramics Monthly. Manufacturer figures are published specifications for the named body at the named cone and do not transfer to other brands. Family ranges are summaries across the sources cited above, not a survey of all clays. Compiled by the Austin Gallery editors, November 2026.

Cite this guide

Writers, framers, designers and students are welcome to quote this page. If you use one number, use this one:

Under the USITC definitions cited in Ceramics Monthly, stoneware absorbs no more than 3 percent of its dry weight in water, porcelain no more than 0.5 percent, and earthenware more than 3 percent.

Suggested citation:

Austin Gallery, "Earthenware vs Stoneware vs Porcelain: The 3 Percent Line," updated November 2026. https://www.austingallery.org/blog/earthenware-vs-stoneware-vs-porcelain

More free charts: the Austin Gallery reference library.