Reference · Updated November 2026
Bisque and glaze firing schedules
The published cone 04 bisque and cone 6 glaze programs, segment by segment in Fahrenheit and Celsius, with the reason each segment is there so you can adjust one without breaking the rest.
By Travis Moher · Published November 17, 2026
A standard slow cone 04 bisque climbs 80°F per hour to 250°F, 200°F per hour to 1000°F, 100°F per hour to 1100°F, 180°F per hour to 1676°F, then 80°F per hour to 1926°F, about 13 hours in all. A slow cone 6 glaze firing climbs 150°F per hour to 250°F, 400°F per hour to 1982°F, then 120°F per hour to 2232°F, about 7.5 hours, with an optional slow cool of 150°F per hour from 2100°F down to 1400°F. These are the Bartlett controller programs and the Plainsman drop-and-hold schedule as published by Tony Hansen at Digitalfire. The witness cone, not the display, decides when the firing is done.
The red-heat rule
The single principle behind every bisque schedule comes from the Orton Ceramic Foundation, the company that makes pyrometric cones: carbon oxidation should be completed below red heat, 1400°F (760°C). Orton puts binder burnoff at 300 to 500°F and the natural carbon in clay at up to 1200 to 1400°F. If the kiln races through that window, carbon stays trapped and shows up later as black coring, bloating, or glaze pinholes. So the bisque is slow where the clay is changing and fast where it is not, and the glaze firing, which starts with clay that has already been through all of this, can climb much faster early on.
Slow cone 04 bisque, segment by segment
This is the Bartlett slow bisque program (Digitalfire code BTSB04). It assumes a start at 75°F (25°C) and uses no holds. It is the right default for most studio ware, and the safe choice whenever you are unsure whether a load is fully dry.
| Segment | Rate | Target | Hold | Elapsed (h:mm) |
|---|---|---|---|---|
| 1 | 80°F/hr (44°C/hr) | 250°F (121°C) | None | 2:11 |
| 2 | 200°F/hr (111°C/hr) | 1000°F (538°C) | None | 5:56 |
| 3 | 100°F/hr (56°C/hr) | 1100°F (593°C) | None | 6:56 |
| 4 | 180°F/hr (100°C/hr) | 1676°F (913°C) | None | 10:08 |
| 5 | 80°F/hr (44°C/hr) | 1926°F (1052°C) | None | 13:15 |
Source: Digitalfire BTSB04. Celsius rates are rate conversions: a change of 100 Fahrenheit degrees is about 55.6 Celsius degrees, which Digitalfire points out is not the same as converting a reading.
What each segment is for
- Segment 1, 80°F/hr to 250°F. Gets every part of every pot past the boiling point of water gently. Free water leaves as steam from 212 to 392°F (100 to 200°C), per Jeff Zamek in Ceramics Monthly. Steam expands to more than 1,500 times the volume of the liquid, which is what bursts a pot.
- Segment 2, 200°F/hr to 1000°F. The organic burnoff window. Finkelnburg puts the start of organic burnout at about 450°F (232°C), and recommends running the kiln vent from there.
- Segment 3, 100°F/hr to 1100°F. The schedule slows down again, on purpose. Chemically bound water leaves the clay between 842 and 1022°F (450 to 550°C), and quartz inversion happens at about 1063°F (573°C). Both put stress on the ware at once.
- Segment 4, 180°F/hr to 1676°F. Through red heat. The risky changes are behind you, and Orton's 1400°F burnout line is crossed at a steady pace.
- Segment 5, 80°F/hr to 1926°F. The slow approach to cone 04. The final temperature is lower than the 1945°F (1063°C) Orton lists for cone 04 at 108°F per hour, because a slower final climb delivers more heat work per degree. Orton's own chart drops cone 04 to 1915°F at 27°F per hour.
Fast cone 04 bisque
The Bartlett fast bisque (BTFB04) has the same shape, with each segment quicker. It finishes at 1945°F because its last segment runs at 108°F per hour, exactly the medium rate in Orton's cone chart. Use it only for thin, fully dry, simple ware you have fired in that clay before.
| Segment | Rate | Target | Hold | Elapsed (h:mm) |
|---|---|---|---|---|
| 1 | 120°F/hr (67°C/hr) | 250°F (121°C) | None | 1:27 |
| 2 | 300°F/hr (167°C/hr) | 1000°F (538°C) | None | 3:57 |
| 3 | 150°F/hr (83°C/hr) | 1100°F (593°C) | None | 4:37 |
| 4 | 180°F/hr (100°C/hr) | 1695°F (924°C) | None | 7:55 |
| 5 | 108°F/hr (60°C/hr) | 1945°F (1063°C) | None | 10:14 |
Source: Digitalfire BTFB04.
Cone 6 glaze firing, segment by segment
A glaze firing starts with bisqueware: the water, carbon, and bound water are already gone, so the early segments can be fast. The care moves to the top of the firing, where the glaze melts and smooths out.
Slow cone 6 glaze (no hold, no controlled cool)
| Segment | Rate | Target | Hold | Elapsed (h:mm) |
|---|---|---|---|---|
| 1 | 150°F/hr (83°C/hr) | 250°F (121°C) | None | 1:10 |
| 2 | 400°F/hr (222°C/hr) | 1982°F (1083°C) | None | 5:30 |
| 3 | 120°F/hr (67°C/hr) | 2232°F (1222°C) | None | 7:35 |
Source: Digitalfire BRTS6, the Bartlett slow glaze program. Digitalfire's own note on it: most kilns reach cone 6 at about 2200°F, not 2232°F. The faster Bartlett cone 6 program (BRTF6) runs 570°F per hour to 1982°F, then 200°F per hour to 2232°F, about 4 hours 35 minutes.
Cone 6 drop-and-hold with slow cool
This is the Plainsman schedule Digitalfire recommends for functional cone 6 ware (C6DHSC). It tops out at 2200°F, drops 100 degrees and soaks for 30 minutes, then cools at a controlled 150°F per hour to 1400°F. Digitalfire credits the controlled cool with better glaze surfaces and recommends the schedule especially for reactive glazes.
| Segment | Rate | Target | Hold | Elapsed (h:mm) |
|---|---|---|---|---|
| 1 | 108°F/hr (60°C/hr) | 250°F (121°C) | 60 min | 2:37 |
| 2 | 350°F/hr (194°C/hr) | 2100°F (1149°C) | 15 min | 8:09 |
| 3 | 108°F/hr (60°C/hr) | 2200°F (1204°C) | 10 min | 9:14 |
| 4 | As fast as possible (down) | 2100°F (1149°C) | 30 min | 9:51 |
| 5 | 150°F/hr (83°C/hr) cooling | 1400°F (760°C) | Off | 14:31 |
Source: Digitalfire C6DHSC. The page advises a longer first hold if the bisque is waterlogged, a faster climb if ware is thin, a slower final climb for thick ware, a longer hold for larger kilns, and setting the top temperature by a self-supporting cone 6.
Witness cones for these schedules
Prices checked November 17, 2026. Affiliate links, so we may earn a commission at no cost to you.
Orton Self-Supporting Cone 04 (25 pack)about $22The witness cone for the bisque on this page. The controller reads temperature; the cone reads heat work, which is what the clay actually responds to.View on Amazon →
Orton Self-Supporting Cone 6 (25 pack)about $20For the glaze firing. Digitalfire calibrates its cone 6 schedules to a self-supporting cone 6, not to the number on the display.View on Amazon →What happens to clay during the bisque
This is the table to keep next to the kiln. Every slow segment in a bisque program lines up with one of these rows. Sources disagree by a few dozen degrees on the edges, so ranges are attributed.
| Stage | Temperature | What it means |
|---|---|---|
| Water smoking | 212 to 392°F (100 to 200°C) | Free water leaves the pores as steam. Jeff Zamek's range, Ceramics Monthly. |
| Organic burnout begins | About 450°F (232°C) | Dave Finkelnburg's starting point. Orton puts binder burnoff at 300 to 500°F. |
| Dehydroxylation | 842 to 1022°F (450 to 550°C) | Chemically bound water leaves the clay crystal. Finkelnburg says it cuts kaolinite's weight by about 13.2%. |
| Quartz inversion | About 1063°F (573°C) | Quartz changes crystal form and volume suddenly, on the way up and again on the way down. |
| Natural carbon burnout ends | Up to 1200 to 1400°F (649 to 760°C) | Orton: oxidation should be completed below red heat, 1400°F. |
Sources: Jeff Zamek, “Techno File: Bisque Firing,” and Dave Finkelnburg, “Bisque Firing 101,” both in Ceramics Monthly; Orton Ceramic Foundation, “Avoiding Carbon Burnout Problems.”
Candling: the step before segment 1
Candling means holding the kiln below the boiling point of water long enough for the last moisture to leave the ware. Finkelnburg describes it as heating as slowly as if the heat source were a candle, and suggests 25°F per hour for 4 to 6 hours as a prudent candle, slower for thick work or ware loaded before it was bone dry. Skutt recommends a 2 hour preheat on any controller that offers one, as insurance against exploding pieces.
The check is simple and worth doing on every doubtful load. With the vent fan off, hold a room-temperature mirror over a vent hole. If it fogs, water is still coming out of the ware, so keep candling. Digitalfire notes that thick sculpture may need days of candling, and gas-fired functional ware is commonly candled overnight on very low heat.
Exceptions and distinctions
- The final temperature is not the cone. A cone measures heat work, which combines temperature and time. That is why the slow bisque stops at 1926°F and the fast one at 1945°F, and why Digitalfire says most kilns reach cone 6 near 2200°F. Our kiln cone temperature chart lists every cone at all three Orton heating rates.
- Air bubbles are not what blows pots up. Sue McLeod's Ceramics Monthly column puts it plainly: only water leads to explosions. Trapped air matters only because it can trap moisture. Candling and segment 1 are the fix, not extra wedging.
- Thick and dense ware needs care on the way down too. Quartz inversion at about 1063°F happens again during cooling. Finkelnburg suggests slowing both heating and cooling around that temperature for kilns loaded with fully dense work.
- A slow cool is a glaze choice, not a safety step. The C6DHSC slow cool from 2100 to 1400°F changes the glaze surface. It can improve one glaze and turn another from gloss to matte, and Digitalfire notes it adds wear on kiln relays.
- Low-fire glaze firings are a different program. Skutt's own instructions for low-fire work are a cone 04 slow bisque, then a cone 06 medium-speed glaze firing, with the lid kept closed until the kiln is below 125°F.
- Bisque cone affects glazing. A cone 06 bisque leaves ware more porous than cone 04, so glaze goes on thicker with the same dip time. Bisque temperature also feeds into final absorption, covered in our clay shrinkage and absorption chart.
Cooling and unloading
Cooling takes about as long as heating. Skutt estimates about 12 hours to cool a slow bisque and a medium glaze firing, depending on kiln size, and says to wait until the kiln is below 125°F before opening the lid. The schedule only ends when the kiln is cool enough to unload, so plan the firing around the cooling time as well as the climb.
Free to use
Put this bisque schedule on your site
Running a community studio or teaching a kiln class? Copy the snippet below to embed the slow cone 04 bisque schedule. It is self-contained and renders anywhere. The only ask is that you keep the small credit link back here.
Click inside the box, select all (⌘A / Ctrl-A), and copy.
Sources
- Tony Hansen, Digitalfire firing schedules: BTSB04, BTFB04, BRTS6, BRTF6, C6DHSC, and the candling glossary entry.
- The Edward Orton Jr. Ceramic Foundation, “Avoiding Carbon Burnout Problems”. Binder and carbon burnout temperatures and the below-red-heat rule.
- Dave Finkelnburg, “Bisque Firing 101,” Ceramics Monthly. Candling rate and mirror test, organic burnout, dehydroxylation, quartz inversion, bisque cone range.
- Jeff Zamek, “Techno File: Bisque Firing,” Ceramics Monthly. Water smoking range and typical bisque cones by clay body.
- Sue McLeod, “Techno File: Air Bubble Myth,” Ceramics Monthly. Steam expansion and why water, not air, causes explosions.
- Skutt Kilns, “Kiln use: how to properly use a kiln”. Cone 04 slow bisque, 2 hour preheat, firing and cooling times, the 125°F unloading rule.
Questions
What is a good slow bisque firing schedule for cone 04?
The Bartlett slow bisque program published by Digitalfire climbs 80°F per hour to 250°F, 200°F per hour to 1000°F, 100°F per hour to 1100°F, 180°F per hour to 1676°F, and 80°F per hour to a final 1926°F (1052°C). It takes about 13 hours 15 minutes to reach temperature, with no holds. Put a cone 04 witness cone in the load, because the cone, not the display, tells you the firing is done.
How long does a bisque firing take?
About 10 to 13 hours to reach cone 04 on standard electric kiln programs, plus about as long again to cool. The Bartlett fast bisque reaches 1945°F in about 10 hours 14 minutes and the slow bisque reaches 1926°F in about 13 hours 15 minutes. Skutt puts a slow cone 04 bisque at about 12 hours up and 12 hours down. Thick work or large sculpture can need 18 hours or more.
Why do you bisque fire slowly below 1000°F?
Because almost everything that can crack or blow up a pot happens below about 1100°F. Free water leaves as steam from 212 to 392°F, organics start burning off around 450°F, chemically bound water leaves between 842 and 1022°F, and quartz changes volume suddenly at about 1063°F (573°C). That is why the slow bisque program drops to 100°F per hour between 1000 and 1100°F before speeding up again.
What is a cone 6 glaze firing schedule?
A common slow cone 6 glaze program climbs 150°F per hour to 250°F, 400°F per hour to 1982°F, then 120°F per hour to 2232°F (1222°C), about 7.5 hours with no hold. Digitalfire's drop-and-hold version runs to 2200°F, holds 10 minutes, drops to 2100°F and holds 30 minutes, then cools at 150°F per hour to 1400°F. Digitalfire notes most kilns reach cone 6 at about 2200°F, so set the final temperature by your witness cone.
What is candling a kiln?
Candling is heating the kiln very slowly, below the boiling point of water, to drive the last moisture out of greenware before the bisque climbs. Dave Finkelnburg suggests 25°F per hour for 4 to 6 hours as a prudent candle, slower for thick work. To check, hold a room-temperature mirror to a vent hole with the vent fan off: if it fogs, water is still leaving the ware.
Should I bisque to cone 06 or cone 04?
Both are standard. Finkelnburg gives cone 08 to 04 as the common bisque range for bodies later glazed at cone 5 and up. Jeff Zamek writes that most stoneware and low-fire bodies are bisqued to cone 06 (1828°F) and porcelain slightly higher, to cone 04 (1945°F). AMACO instructs applying its glazes to cone 04 bisque. A cooler bisque leaves the ware more porous, so it absorbs glaze faster.
Does a slow cool help cone 6 glazes?
Often, but not always in the direction you want. Digitalfire's C6DHSC schedule cools at 150°F per hour from 2100°F to 1400°F and credits the slow cool with better glaze surfaces, but the same page notes it can turn some glossy glazes matte. Digitalfire also notes slow cools can shorten relay life in electric kilns. Test a glaze on a tile with the schedule before committing a whole load.
Are these affiliate links?
Some are. Austin Gallery is an Amazon affiliate, so if you buy through a product link here Amazon pays us a small commission at no extra cost to you. Every schedule on this page is attributed to the source that publishes it. See our full affiliate disclosure.
Keep reading
- The kiln cone temperature chart: every Orton cone in °F and °C at all three heating rates.
- Clay shrinkage and absorption rates: what the glaze firing does to the size and porosity of the pot.
- The best electric kilns for home use: which controllers can run custom segments like these.
- Kiln electrical requirements: the circuit a cone 6 kiln needs before any of this matters.
Segment tables reproduce the programs published by Digitalfire under the codes shown. Elapsed times are calculated from the published rates and targets from a 75°F start. Temperatures for clay changes are attributed to Ceramics Monthly and Orton as cited above. Every kiln fires differently: confirm each schedule with witness cones in your own kiln before relying on it. Compiled by the Austin Gallery editors, November 2026. Austin Gallery may earn a commission from product links on this page at no cost to you.
Cite this guide
Writers, framers, designers and students are welcome to quote this page. If you use one number, use this one:
A standard slow cone 04 bisque takes about 13 hours and climbs no faster than 200°F per hour until it passes 1100°F.
Suggested citation:
Austin Gallery, "Bisque and Glaze Firing Schedules: Cone 04 and Cone 6, Segment by Segment," updated November 2026. https://www.austingallery.org/blog/bisque-and-glaze-firing-schedules
More free charts: the Austin Gallery reference library.